A high strength alloy with, dependent upon temper, minimum Proof Stress up to 56 ksi / 385 Mpa and minimum Tensile Strength up to 70 ksi / 482 MPa
SAE AMS QQ-A-200/3 Alloy QQ-A-200/3 |
|
---|---|
Chemical Element | % Present |
Aluminium (Al) | balance |
Other (Each) | 0.05 max |
Chromium (Cr) | 0.1 max |
Titanium (Ti) | 0.15 max |
Others (Total) | 0.15 max |
Zinc (Zn) | 0.25 max |
Silicon (Si) | 0.5 max |
Iron (Fe) | 0.5 max |
Manganese (Mn) | 0.3 - 0.9 |
Magnesium (Mg) | 1.2 - 1.8 |
Copper (Cu) | 3.8 - 4.9 |
Aluminium alloy QQ-A-200/3 has similarities to the following standard designations and specifications:
AMS 4164, AMS 4165
Alloy QQ-A-200/3 is supplied in a range of tempers:
Alloy QQ-A-200/3 is supplied as Extruded Bar
Physical Property | Value |
---|---|
Density | 2.74 g/cm³ |
Melting Point | 640 °C |
Thermal Expansion | 23.1 x10^-6 /K |
Modulus of Elasticity | 73 GPa |
Thermal Conductivity | 121 W/m.K |
Electrical Resistivity | 30 % IACS |
These apply to QQ-A-200/3 bar in the T3 temper
Diameter (mm) | Proof Strength (Min) | Tensile Strength (Min) | Elongation % (Min) |
Up to & incl. 6.25mm | 290 | 393 | 12 |
Over 6.3mm up to & incl. 19mm | 303 | 414 | 12 |
Over 19mm up to & incl. 38mm | 317 | 448 | 10 |
Over 38mm | 358 | 483 | 10 |