A medium to high strength alloy with, dependent upon temper, minimum Proof Stress up to 57 ksi / 390 Mpa and minimum Tensile Strength up to 66 ksi / 455 MPa
SAE AMS QQ-A-250/4 Alloy QQ A 250/4 |
|
---|---|
Chemical Element | % Present |
Aluminium (Al) | balance |
Other (Each) | 0.05 max |
Chromium (Cr) | 0.1 max |
Titanium (Ti) | 0.15 max |
Others (Total) | 0.15 max |
Titanium + Zirconium (Ti+Zr) | 0.2 max |
Zinc (Zn) | 0.25 max |
Silicon (Si) | 0.5 max |
Iron (Fe) | 0.5 max |
Manganese (Mn) | 0.3 - 0.9 |
Magnesium (Mg) | 1.2 - 1.8 |
Copper (Cu) | 3.8 - 4.9 |
Aluminium alloy QQ-A-250/4 has similarities to the following standard designations and specifications but may not be a direct equivalent:
AMS 4035, Alloy 2024, UNS A92024
Alloy QQ-A-250/4 is supplied in a wide range of tempers: T351 is intended to provide material with low residual stresses and thus minimal distortion during machining, but does not provide optimal corrosion resistance.
Alloy QQ-A-250/4 T351 s supplied in plate and sheet
Physical Property | Value |
---|---|
Density | 2.79 g/cm³ |
Melting Point | 640 °C |
Thermal Expansion | 23.1 x10^-6 /K |
Modulus of Elasticity | 73 GPa |
Thermal Conductivity | 121-150 W/m.K |
Electrical Resistivity | 30-40 % IACS |
The Mechanical Properties given are for Plate in the T351 temper.
Thickness (mm) | Proof Strength (Min) | Tensile strength (Min) | Elongation % (Min) |
Over 6.6 up to & incl. 12.6 | 290 | 441 | 12 |
12.7 up to & incl. 25.4 | 290 | 434 | 8 |
Over 25.4 up to & incl. 38.1 | 290 | 427 | 7 |
Over 38.1 up to & incl. 50.8 | 290 | 427 | 6 |
Over 50.8 up to & incl. 76.2 | 290 | 414 | 4 |
Over 76.2 up to & incl. 101.6 | 283 | 393 | 4 |